常见的精密铸造缺陷

RELEASE TIME :

2019-10-09 07:59

常见的精密铸造缺陷有气泡,气泡是指精细铸件个别位置呈现润滑孔眼缺陷。气泡通常在机加工之后才干被发现。我们的精密铸造技术人员分离多年车间消费经历,对精密铸造中呈现气泡的缘由及预防办法总结如下:

一、构成缘由:
1.大多数状况下呈现气泡主要是由于精细铸外型壳焙烧不充沛,浇注钢水时型壳霎时产生大量气体无法顺利排出,进而侵入金属液中构成气泡;
2.由于制壳工艺或壳型资料缘由,型壳透气性太差,型腔中气体难以排出,进入金属液中构成气泡;
3.浇注时卷入钢水中的空气未能排出从而形成的铸件气泡。

二、预防办法
1.在精密铸造条件允许的状况下,在构造复杂的铸件高处设置排气泡。
2.在设计浇注系统时,要充沛思索到型壳排气需求。
3.型壳焙烧温度、时间要合理,保温时间也要充足。
4.脱蜡时应将蜡料彻底扫除。
5.恰当降低浇包嘴到浇口杯间隔,浇注速度要平均,以确保钢程度稳充溢型腔,尽可能少的卷入钢水中空气,以便型腔中及钢水中气体能顺利排出

RELATED NEWS

Japanese businessmen come to our mingxing foundry company for inspection

On March 25, Japanese businessmen came to our mingxing foundry company for inspection, and spoke highly of the quality of our products. The picture shows feng xianyuan, general manager of mingxing foundry and company leaders accompanying and introducing the company's products and company development.

2019/02/28 15:08

Responsible person for Israel to introduce products

The picture shows that the leaders of the company are introducing the company's products and future development to Israeli customers

2019/02/28 15:07

American businessmen visit the production site

The picture shows the leaders of the company introducing the company's products to American businessmen

2019/02/28 15:06

< 1234 >